10−1 to 103 HzM33 > 10−18 m2 V−2,
all compositions
Steady across four decades of frequency
Every calcium-doped composition holds a high, flat electrostrictive coefficient from 0.1 Hz to 1 kHz. Trivalent-doped ceria, by contrast, loses most of its response above about 1 to 10 Hz, a sign of slow, coupled electro-chemo-mechanical processes.
1 VO per Ca2+vs one per two Gd3+
A different kind of defect
A divalent dopant needs one oxygen vacancy for charge balance, so each Ca2+ comes with its own vacancy. The authors trace the frequency-stable response to strong electro-steric interactions within these Ca2+–vacancy pairs, a form of electromechanical coupling distinct from the slow elastic dipoles of trivalent-doped ceria.
x = 0.025–0.15grains 3.0–4.8 µm;
CaO at boundaries for x = 0.15
Insensitive to composition and microstructure
Nominal vacancy concentration, CaO segregation and microstructure change M33 only slightly. At the highest calcium content a Ca-rich secondary phase collects at grain boundaries and triple junctions without spoiling the response.
Less anelasticthan Gd-doped ceria
(nanoindentation creep)
Mechanically quieter
All compositions show primary creep at room temperature, linked to reorientation of vacancy-related complexes under stress. Creep is suppressed for intermediate calcium contents and rises again at x = 0.15. Overall the calcium-doped ceramics are less anelastic than 10 mol% Gd-doped ceria, and their elastic moduli fall as calcium increases.
≈ 0.85 eVbulk activation energy,
≈ 1.10 eV grain boundary
Still a good oxide-ion conductor
Except at the lowest doping, total ionic conductivity is close to that of Gd-doped ceria, and the activation energies hardly change with calcium content. The Ca-rich boundary phase does not significantly reduce the conductivity.